Ratings are given for standard seamless pipe sizes at temperatures from 100oF to 750oF. All ratings are in psig based on ANSI/ASME B 31.1.
| Maximum Allowable Pressure (psig) | ||||||||||
| Pipe Size (inches) | Pipe Schedule | Temperature (oF) | ||||||||
| 100 | 200 | 300 | 400 | 500 | 600 | 650 | 700 | 750 | ||
| 1" | 401) | 2857 | 2857 | 2857 | 2857 | 2857 | 2857 | 2857 | 2743 | 2476 |
| 802) | 3950 | 3950 | 3950 | 3950 | 3950 | 3950 | 3950 | 3792 | 3423 | |
| 160 | 5757 | 5757 | 5757 | 5757 | 5757 | 5757 | 5757 | 5526 | 4989 | |
| 1 1/2" | 40 | 2116 | 2116 | 2116 | 2116 | 2116 | 2116 | 2116 | 2032 | 1834 |
| 80 | 2983 | 2983 | 2983 | 2983 | 2983 | 2983 | 2983 | 2864 | 2585 | |
| 160 | 4331 | 4331 | 4331 | 4331 | 4331 | 4331 | 4331 | 4157 | 3753 | |
| 2" | 40 | 1783 | 1783 | 1783 | 1783 | 1783 | 1783 | 1783 | 1712 | 1545 |
| 80 | 2575 | 2575 | 2575 | 2575 | 2575 | 2575 | 2575 | 2472 | 2232 | |
| 160 | 4217 | 4217 | 4217 | 4217 | 4217 | 4217 | 4217 | 4049 | 3655 | |
| 3" | 40 | 1693 | 1693 | 1693 | 1693 | 1693 | 1693 | 1693 | 1625 | 1467 |
| 80 | 2394 | 2394 | 2394 | 2394 | 2394 | 2394 | 2394 | 2298 | 2074 | |
| 160 | 3600 | 3600 | 3600 | 3600 | 3600 | 3600 | 3600 | 3456 | 3120 | |
| 4" | 40 | 1435 | 1435 | 1435 | 1435 | 1435 | 1435 | 1435 | 1378 | 1244 |
| 80 | 2075 | 2075 | 2075 | 2075 | 2075 | 2075 | 2075 | 1992 | 1798 | |
| 160 | 3376 | 3376 | 3376 | 3376 | 3376 | 3376 | 3376 | 3241 | 2926 | |
| 5" | 40 | 1258 | 1258 | 1258 | 1258 | 1258 | 1258 | 1258 | 1208 | 1090 |
| 80 | 1857 | 1857 | 1857 | 1857 | 1857 | 1857 | 1857 | 1783 | 1610 | |
| 160 | 3201 | 3201 | 3201 | 3201 | 3201 | 3201 | 3201 | 3073 | 2774 | |
| 6" | 40 | 1143 | 1143 | 1143 | 1143 | 1143 | 1143 | 1143 | 1098 | 991 |
| 80 | 1794 | 1794 | 1794 | 1794 | 1794 | 1794 | 1794 | 1722 | 1554 | |
| 160 | 3083 | 3083 | 3083 | 3083 | 3083 | 3083 | 3083 | 2960 | 2672 | |
| 8" | 40 | 1006 | 1006 | 1006 | 1006 | 1006 | 1006 | 1006 | 966 | 872 |
| 80 | 1586 | 1586 | 1586 | 1586 | 1586 | 1586 | 1586 | 1523 | 1375 | |
| 160 | 2976 | 2976 | 2976 | 2976 | 2976 | 2976 | 2976 | 2857 | 2579 | |
| 10" | 40 | 913 | 913 | 913 | 913 | 913 | 913 | 913 | 876 | 791 |
| 80 | 1509 | 1509 | 1509 | 1509 | 1509 | 1509 | 1509 | 1448 | 1308 | |
| 160 | 2950 | 2950 | 2950 | 2950 | 2950 | 2950 | 2950 | 2832 | 2557 | |
1) STD (standard) = schedule 40
2) XS (extra strong) = schedule 80