Dimensions and working pressure of copper tubes according BS 2871:1972 can be found in the table below:
| Nominal bore (mm) | Outside Diameter (mm) | Table X Half hard light gauge tube | Table Y Half hard an annealed tube | Tabel Z Hard drawn thin wall tube | |||
| Thickness (mm) | Maximum working pressure (N/mm2) | Thickness (mm) | Maximum working pressure (N/mm2) | Thickness (mm) | Maximum working pressure (N/mm2) | ||
| 6 | 6 | 0.6 | 13.3 | 0.8 | 14.4 | 0.5 | 11.3 |
| 8 | 8 | 0.6 | 9.7 | 0.8 | 10.5 | 0.5 | 9.8 |
| 10 | 10 | 0.6 | 7.7 | 0.8 | 8.2 | 0.5 | 7.8 |
| 12 | 12 | 0.6 | 6.3 | 0.8 | 6.7 | 0.5 | 6.4 |
| 15 | 15 | 0.7 | 5.8 | 1 | 6.7 | 0.5 | 5 |
| 18 | 18 | 0.8 | 5.6 | 1 | 5.5 | 0.6 | 5 |
| 22 | 22 | 0.9 | 5.1 | 1.2 | 5.7 | 0.6 | 4.1 |
| 28 | 28 | 0.9 | 4 | 1.2 | 4.2 | 0.6 | 3.2 |
| 35 | 35 | 1.2 | 4.2 | 1.5 | 4.1 | 0.7 | 3 |
| 42 | 42 | 1.2 | 3.5 | 1.5 | 3.4 | 0.8 | 2.8 |
| 54 | 54 | 1.2 | 2.7 | 2 | 3.6 | 0.9 | 2.5 |
| 67 | 67 | 1.2 | 2 | 2 | 2.8 | 1 | 2 |
| 76.1 | 76.2 | 1.5 | 2.4 | 2 | 2.5 | 1.2 | 1.9 |
| 108 | 108.1 | 1.5 | 1.7 | 2.5 | 2.2 | 1.2 | 1.7 |
| 133 | 133.4 | 1.5 | 1.4 | 1.5 | 1.6 | ||
| 159 | 159.4 | 2 | 1.5 | 1.5 | 1.5 | ||