Copper Zinc Tin Alloys

Strength of Copper-Zinc-Tin alloys

Tensile strength of copper-zinc-tin alloys are indicated below:

Copper
(%)
Zinc
(%)
Tin
(%)
Tensile Strength
(105 kPa) (lb/in2)
45 50 5 1.03 15000
50 45 5 3.45 50000
50 40 10 1.03 15000
55 43 2 4.48 65000
55 40 5 4.27 62000
55 35 10 2.24 32500
55 30 15 1.03 15000
60 37 3 4.14 60000
60 35 5 3.62 52500
60 30 10 2.76 40000
60 20 20 0.69 10000
65 30 5 3.45 50000
65 25 10 2.9 42000
65 20 15 2.1 30000
65 15 20 1.24 18000
65 10 25 0.83 12000
70 25 5 3.1 45000
70 20 10 3.03 44000
70 15 15 2.55 37000
70 10 20 2.1 30000
75 20 5 3.1 45000
75 15 10 3.1 45000
75 10 15 2.96 43000
75 5 20 2.8 41000
80 15 5 3.1 45000
80 10 10 3.1 45000
80 5 15 3.3 47500
85 10 5 3 43500
85 5 10 3.2 46500
90 5 5 2.9 42000

Search the Engineering Toolbox

Related Topics

  • Material Properties - Material properties - density, heat capacity, viscosity and more - for gases, fluids and solids

Related Documents

ToolBox Tools

3D Engineering ToolBox - draw and model technical applications! 3D Engineering ToolBox - 3D modelling of technical applications with Google SketchUp!

2D Engineering ToolBox - create and share online diagram drawing templates! 2D Engineering ToolBox - create and share online diagram drawings with Google Docs!

Engineering ToolBox Apps - mobile online and offline engineering applications! Engineering ToolBox Apps - mobile online and offline engineering applications!

Disclaimers

The content in The Engineering ToolBox is COPYRIGHTED but can be used with NO WARRANTY or LIABILITY

Important information should always be double checked with alternative sources. All applicable national and local regulations and practices concerning this aspects must be strictly followed and adhered to. Contact Us!


Desktop Edition!