Resources, Tools and Basic Information for Engineering and Design of Technical Applications!

Resources, Tools and Basic Information for Engineering and Design of Technical Applications!

mobile - visible on handheld devices - alternatively go to www.engineeringtoolbox.com!

Engineering ToolBox > Polypropylene PP and Chemical Resistance

Chemical resistance of polypropylene - PP - to some common acids, bases, organic substances and solvents

The chemical resistance of polypropylene to some common products and chemicals can be found in the tables below:

Acids and Polypropylene

Product Rating 1)
20oC 60oC
Benzoic acid 1 2
Boric acid 1 1
Hydrobromic acid 25 % 2 3
Citric acid 1 1
Hydrocyanic acid 2 2
Hydrofluoric acid 2 2
Phosphoric acid 25 % 1 1
Phosphoric acid 85 % 1 1
Phthalic acid 1 1
Tannic acid 1 1
Chromic acid 1 2
Maleic acid 1 1
Oleic acid 2 3
Oxalic acid 1 1
Nitric acid 5 % 2 3
Nitric acid 65 % 4 4
Chlorhydric acid 10 % 1 1
Chlorhydric acid 37 % 2 3
Butyric acid 1 1
Sulphuric acid 10 % 1 1
Sulphuric acid 78 % 2 4
Sulphuric acid 93 % 3 4
Tartaric acid 1 1
Acetic acid 10 % 1 1
Acetic acid 50 % 1 1
Acetic acid 75 % 1 1
Acetic acid 100 % 2 3
Perchloric acid 1 2

Bases and Polypropylene

Product Rating 1)
20oC 60oC
Aqua ammonia 1 1
Calciumhydroxide 1 1
Potassiumhydroxide 1 1
Caustic soda 1 1
Acid salt 2) 1 1
Basic salt 3) 1 1
Neutral salt 4) 1 1
Various salt
Potassium bicarbonate 1 2
Potassium permanganate 1 2
Sodium cyanide 1 1
Natriumferricyanid 1 2
Sodium hypochlorite 2 3

Organic Substances, Solvents and Polypropylene

Product Rating 1)
20oC 60oC
Acetone 3 4
Aniline 1 1
Benzol 3 4
Petrol 4 4
Butyl alcohol 1 1
Ethyl acetate 2 4
Ethyl alcohol 1 1
Ethyl dichloride 3 4
Ethyl ether 4 4
Phenol 2 2
Formalin 37% 1 2
Heptanes 3 4
Chlorobenzene 3 4
Chloroform 4 4
Carbon disulphide 4 4
Carbon tetrachloride 4 4
Methyl alcohol 1 1
Methylene (di)chloride 4 4
Methyl ethyle ketone 3 4
Nitrobenzene 3 4
Toluene 3 4
Trichlorethylene 4 4
Gases
Chlorine (damp) 2 4
Chlorine (dry) 2 4
Carbon dioxide 1 1
Carbon monoxide 1 1
Sulphur dioxide (damp) 2 3
Sulphur dioxide (dry) 2 3
Hydrogen sulphide 1 1

1) Rating:

  1. Excellent (no attack)
  2. Good (no significant attack)
  3. Acceptable (light attack, limited use)
  4. Unacceptable (significant attack)
  5. Inferior (possible cracking or dissolving)

2) Acid salt (normally aqueous) aluminum chloride, aluminum phosphate, copper chloride, sulphate of copper, ferrous sulphate, ferric chloride, stannic chloride, chloride of zinc, white vitriol etc

3) Basic salt (normally aqueous) bicarbonate of potassium, potash, sodium bicarbonate, sodium carbonate, sodium phosphate etc.