Mechanical properties for some aluminum alloys are indicated below:

Alloy Temper Elastic Modulus
- E -
(106 psi)
Shear Modulus
- G -
(106 psi)
Yield Strength
(103 psi)
Tensile Strength
(103 psi)
1100   10.0 3.75 3.5 11
1100 H12 10.0 3.75 11 14
2014   10.8 4.00 8 22
2014 T6 10.6 4.00 58 66
2014 T62 10.8 4.00 59 67
2017 T4 10.5 3.95 32 55
2024 T3 10.6 4.00 42 64
2024 T4 10.6 4.00 40 62
2025 T6 10.4 3.90 33 52
2124 T851 10.4 4.00 57 66
2219 T62 10.5 4.00 36 54
2618 T61 10.7 4.10 42 55
3003   10.0 3.75 5 14
3003 H18 10.0 3.75 25 27
3003 H112 10.0 3.75 10 17
354 T61 10.6 4.00 36 47
355 T51 10.2 3.80 22 27
355 T6 10.3 3.80 23 37
356 T7 10.3 3.85 21 29
356 T6 10.3 3.85 20 30
5052   10.2 3.80 9.5 25
5052 H32 10.2 3.80 23 31
5056 H38 10.3 3.75 50 60
5056 ANL 10.3 4.00 22 42
6061 T4 10.0 3.80 16 30
6061 T6 10.0 3.80 35 42
6062   10.0 3.75 5 14
6062 T4 10.0 3.75 16 26
6062 T6 10.0 3.75 35 38
6063 T42 10.0 3.75 10 17
6063 T5 10.0 3.75 16 22
6063 T6 10.0 3.75 25 30
6151 T6 10.1 3.85 37 44
7075 T6 10.4 3.90 70 78
A356 T61 10.4 3.90 28 38
D712 T5 10.3 3.80 20 32

Search the Engineering Toolbox

Related Topics

  • Codes and Standards - Piping codes and standards - ASME, ANSI, ASTM, AGA, API, AWWA, BS, ISO, DIN and more..

Related Documents

ToolBox Tools

3D Engineering ToolBox - draw and model technical applications! 3D Engineering ToolBox - 3D modelling of technical applications with Google SketchUp!

2D Engineering ToolBox - create and share online diagram drawing templates! 2D Engineering ToolBox - create and share online diagram drawings with Google Docs!

Engineering ToolBox Apps - mobile online and offline engineering applications! Engineering ToolBox Apps - mobile online and offline engineering applications!

Disclaimers

The content in The Engineering ToolBox is COPYRIGHTED but can be used with NO WARRANTY or LIABILITY

Important information should always be double checked with alternative sources. All applicable national and local regulations and practices concerning this aspects must be strictly followed and adhered to. Contact Us!


Desktop Edition!