| Alloy | Temper | Elastic Modulus - E - 106 (psi) | Shear Modulus - G - 106 (psi) | Yield Strength 103 (psi) | Tensile Strength 103 (psi) |
| 1100 | 10.0 | 3.75 | 3.5 | 11 | |
| 1100 | H12 | 10.0 | 3.75 | 11 | 14 |
| 2014 | 10.8 | 4.00 | 8 | 22 | |
| 2014 | T6 | 10.6 | 4.00 | 58 | 66 |
| 2014 | T62 | 10.8 | 4.00 | 59 | 67 |
| 2017 | T4 | 10.5 | 3.95 | 32 | 55 |
| 2024 | T3 | 10.6 | 4.00 | 42 | 64 |
| 2024 | T4 | 10.6 | 4.00 | 40 | 62 |
| 2025 | T6 | 10.4 | 3.90 | 33 | 52 |
| 2124 | T851 | 10.4 | 4.00 | 57 | 66 |
| 2219 | T62 | 10.5 | 4.00 | 36 | 54 |
| 2618 | T61 | 10.7 | 4.10 | 42 | 55 |
| 3003 | 10.0 | 3.75 | 5 | 14 | |
| 3003 | H18 | 10.0 | 3.75 | 25 | 27 |
| 3003 | H112 | 10.0 | 3.75 | 10 | 17 |
| 354 | T61 | 10.6 | 4.00 | 36 | 47 |
| 355 | T51 | 10.2 | 3.80 | 22 | 27 |
| 355 | T6 | 10.3 | 3.80 | 23 | 37 |
| 356 | T7 | 10.3 | 3.85 | 21 | 29 |
| 356 | T6 | 10.3 | 3.85 | 20 | 30 |
| 5052 | 10.2 | 3.80 | 9.5 | 25 | |
| 5052 | H32 | 10.2 | 3.80 | 23 | 31 |
| 5056 | H38 | 10.3 | 3.75 | 50 | 60 |
| 5056 | ANL | 10.3 | 4.00 | 22 | 42 |
| 6061 | T4 | 10.0 | 3.80 | 16 | 30 |
| 6061 | T6 | 10.0 | 3.80 | 35 | 42 |
| 6062 | 10.0 | 3.75 | 5 | 14 | |
| 6062 | T4 | 10.0 | 3.75 | 16 | 26 |
| 6062 | T6 | 10.0 | 3.75 | 35 | 38 |
| 6063 | T42 | 10.0 | 3.75 | 10 | 17 |
| 6063 | T5 | 10.0 | 3.75 | 16 | 22 |
| 6063 | T6 | 10.0 | 3.75 | 25 | 30 |
| 6151 | T6 | 10.1 | 3.85 | 37 | 44 |
| 7075 | T6 | 10.4 | 3.90 | 70 | 78 |
| A356 | T61 | 10.4 | 3.90 | 28 | 38 |
| D712 | T5 | 10.3 | 3.80 | 20 | 32 |